Aumento en la fuerza de adhesión a dentina con una capa extra de adhesivo dentinal
The purpose of this study was to evaluate if the bonding strength of dentin to dentin bonding agents increases with the application of a third layer of adhesive. 30 extracted molars were cut and embedded in acrylic before having the mid-dentin exposed with 600 grit SiC paper. Adhesives Prime&Bond NT, SingleBond 2 and Excite were applied, one group (n=5) received two layers of adhesive, as indicated by the manufacturer, and another group received a third layer of adhesive. Samples were stored in water for 7 days at 37º C before being tested in shear at a speed of 1 mm/min. Results in MPa were: PBNT 2 layers: 19.3; PBNT 3 layers: 32.6; SB2, 2 layers: 32.1; 3 layers: 38.2; EXC 2 layers: 38.2; lication of athird layer of adhesive increases the bond strength on dentin of the dentin bonding agents used in this study.